When a product must be water- and air-tight, positioning and the ultrasonic energy director are the keys to success. Product design must therefore consider positioning, material, wall thickness, and their proportions relative to the energy director — they are absolutely interrelated. For general water/air-tight requirements, the energy director height should be in the range of 0.5~0.8 m/m (depending on product wall thickness). Below 0.5 m/m, water/air-tightness cannot be achieved unless positioning is extremely precise and wall thickness is at least 5 m/m; otherwise results will be poor.
Common positioning and energy-director designs for water/air-tight products are as follows:
Bevel (scarf) joint: suitable for water-tight and large-part welding, contact face angle =45°, x=w/2, d=0.3~0.8 mm is ideal.
Stepped point: suitable for water-tightness and for preventing external flash or cracking, contact face angle= 45°, x=w/2, d=0.3~0.8 mm is ideal.
Peak-and-valley point: suitable for water-tight, high-strength welding, d=0.3~0.6 mm; the height h of the inner contact face varies with geometry, but h is generally about 1~2 mm.
※ The above are three energy-director designs for water/air-tight ultrasonic welding.
Problem 2: improper welding conditions
When ultrasonic welding fails to achieve water/air-tightness, causes include the energy director, fixture positioning, and the product's own positioning — but the ultrasonic parameter settings are also a major factor. Here we examine the other cause affecting water/air-tightness (welding conditions) more deeply. In ultrasonic welding, speed and efficiency are the most basic goals, but people often miss the key to achieving that efficiency. We will discuss it from two conditions below:
1. Downstroke speed and cushioning too fast: this forming speed causes dynamic pressure plus gravitational acceleration to flatten the energy director, so it cannot perform its energy-directing function, producing a false (apparent) weld.
2. Weld time too long: the plastic part absorbs heat for too long, which not only melts the plastic material but carbonizes the plastic structure, creating porosity (sand holes) through which water or air seeps out. This is the hardest thing for most production technicians to spot,