An ultrasonic welding machine generally runs at either 20 kHz or 40 kHz, with 20 kHz units being more common.
    Joint design: the first and most common joint type uses ultrasonic vibration perpendicular to the mating surfaces. Butt joints and Z-joints fall into this category and suit most polymers. The second type of ultrasonic weld joint uses vibration parallel to the joint surfaces, creating a shear condition. Shear and interference joints of this type fall into the second category, and energy-control 嚣 joints work best with amorphous materials.
    Flash can be reduced to safe levels by introducing flash traps into the joint design; a typical flash trap design provides at least 10% excess volume capacity.
    *Interference joints: to minimize flash formation, interference joints are designed to block the melt or keep it within the melt zone. Interference joints are useful for semi-crystalline plastics such as nylon. Because the joint structure is more complex, interference joints require relatively tight part fit tolerances. Compared with triangular energy-director welds, the larger joint structure also requires additional amplitude and weld energy.
    Part alignment: a simple butt joint does nothing to align or center the parts; alignment is better achieved with molded locating pins or studs. Z-joints self-align, resist tension in use, improve shear-load performance, and eliminate external flash.
    *Tongue-and-groove joints provide both shear and tensile strength. This joint is self-centering; the wall thickness at the joint area must be relatively large to accommodate the tongue-and-groove design. Part tolerances are also relatively tight, and spaced stiffening ribs improve joint alignment.
    When joint quality is good, shear joints are generally recommended. Ring- and rectangular-shaped parts requiring high-strength, high-quality joints all use shear joints. Shear joints have overlapping part walls; when the joint is welded and the parts telescope into each other, the overlapping sections create tolerance and localized shear. To aid part alignment, the joint includes an adjusting section. To concentrate melting energy, the apex of a stop on one side is reduced at the initial contact surface. Because the molten material's temperature stays consistent across the entire contact surface, the two surfaces melt uniformly as the part is welded. For depths of 1.0-2.0 mm, tolerance values in the 0.13-0.5 mm range are used. To prevent external side-wall warping caused by tolerances during welding, vertical parts should be as shallow as possible; but a shear-assisted tongue-and-groove joint on one side can be used with deeper drawn parts, providing an intermediate wall joint that minimizes tolerance-induced side-wall warping.
A scarf joint has an angle of 30°-60° and should be assembled within ±1°. A tolerance of 0.10-0.25 mm added for the additional melt-zone material thickness produces the weld and flash. When flash is unacceptable for functional or cosmetic reasons, a collector is used.