Ultrasonic Welding:
The most common method of welding thermoplastic parts is ultrasonic welding. It uses low-amplitude, high-frequency (ultrasonic) vibration energy to generate, through surface and molecular friction, the heat needed to weld the mating plastic parts. (Sinusoidal ultrasonic vibration)
Ultrasonic welding takes place in the 20–50 kHz frequency range, with typical amplitudes of 15–60 µm. Sonic frequencies as low as 15 kHz (at higher amplitudes) are sometimes used for larger parts or softer materials. The weld cycle usually lasts 0.5–1.5 s. Weld process variables include weld time, horn position, and weld pressure. Ultrasonic welding equipment is generally used for small and medium-sized thermoplastic parts, while very large parts can be joined with multi-point welding.
Ultrasonic welding can be controlled by weld time, weld position (collapse distance), or weld energy. Additional control of weld pressure and cooling time is also available.
Ultrasonic welding equipment generally operates at either 20 kHz or 40 kHz. 20 kHz systems are more common.
Joint design: the first and most common joint type uses ultrasonic vibration perpendicular to the surfaces being joined. Butt joints and Z-joints fall into this category and suit most polymers. The second type of ultrasonic weld joint uses vibration parallel to the joint surfaces, creating a shear condition; various shear and interlocking joints belong to this second type.
Energy director joints work best with amorphous materials; larger energy directors can be used in some unsealed semi-crystalline materials. A rough or textured surface on the part below improves the joint. This increases weld quality, weld strength, and ease of welding. Many other textured joint profiles are also viable.
Flash problems can be reduced by incorporating a flash trap into the joint design; for safety, flash traps are generally designed with at least 10% excess volume capacity.
Interference joints: to minimize the likelihood of flash, interference joints are designed to block the melt or keep it within the melt zone. Interference joints are useful for semi-crystalline plastics such as nylon. Because the joint geometry is more complex, interference joints require relatively tight part fit tolerances. Compared with triangular energy director welding, the larger joint geometry also demands additional amplitude and weld energy.
Part Alignment A simple butt joint provides no means of aligning or centering the parts. Alignment is better achieved with molded locating pins or double-ended studs. Z-joints self-align, resist tension in use, improve shear load resistance, and eliminate external flash.
Tongue-and-groove joints provide both shear and tensile strength. This joint is self-aligning, but the wall thickness in the joint area must be relatively large to accommodate the tongue-and-groove design. Part tolerances are also relatively tight. Spacer ribs improve joint alignment.
When designing joints, shear joints are generally recommended — use shear joints. Ring-shaped and rectangular parts requiring high-strength, high-quality joints all use shear joints. Shear joints feature overlapping wall sections of the parts; as the joint is welded and the parts telescope together, the overlapping sections create interference and localized shear. To promote part alignment, the joint includes an alignment feature. To concentrate the melting energy, the apex of the barrier on one side is reduced at the initial contact surface. Because the molten material stays at a consistent temperature across the whole contact face, both surfaces melt uniformly as the parts are welded. For depths of 1.0–2.0 mm, tolerances in the range of 0.13–0.5 mm are used. To prevent external sidewall warping caused by tolerances during welding, vertical parts should be kept as shallow as possible; however, a tongue-and-groove joint modified with a shear part on one side can be used with deeper drawn parts to provide an intermediate-wall joint that minimizes tolerance-induced sidewall warping.
Scarf joints have an angle of 30°–60° and should be assembled within ±1°. A 0.10–0.25 mm tolerance added to the melt-zone material thickness produces the weld and the flash. When flash is unacceptable for functional or cosmetic reasons, a flash trap is used. Welding with an embedded seal Reliable sealing can also be achieved with an embedded elastomeric seal or resilient gasket. As shown in Fig. 7, the joint part carries an elastic ring to improve the sealing reliability achievable with ultrasonic welding, or for use where continuous peripheral welding is not possible.